Hashin Damage in Abaqus: Setup, Inputs and Fixes

Hashin Damage in Abaqus: Setup, Inputs and Fixes

Table of Contents

You add Hashin damage to a composite model, run it, and one of two things usually happens. Either the job finishes with no damage anywhere, or it stops a few increments after the first element starts to fail. Both are normal first attempts, and both come from the same place: Hashin damage in Abaqus is a two-part model, and most of the real work sits in the second part.

This guide covers what the model does, the exact inputs it needs, which element types support it, and how to get past the convergence wall that stops most first attempts.

What Hashin damage does in Abaqus

Hashin damage is a continuum damage model for a fibre-reinforced lamina. It works ply by ply, in the material coordinate system, where direction 1 is the fibre direction and direction 2 is transverse to the fibres. It does not smear the laminate into one equivalent material, and it does not look at the interfaces between plies.

The model runs in two stages:

  • Damage initiation — tells the solver when damage starts in each failure mode. This alone changes nothing about stiffness. It only sets flags.
  • Damage evolution — tells the solver how fast stiffness drops after initiation. This is what actually softens the material and produces a load drop.

Define initiation but skip evolution and your model will report that everything failed while the load-displacement curve keeps climbing. That is the single most common reason people say “Hashin is not working”.

The four failure modes

Abaqus evaluates four criteria in effective stress space, following Hashin and Rotem (1973) and Hashin (1980):

  • Fibre tension
  • Fibre compression
  • Matrix tension
  • Matrix compression

Each mode has its own damage variable, strength input and fracture energy, and each degrades a different stiffness term. So a ply can lose all transverse stiffness while the fibres still carry load — exactly the behaviour you want in a laminate. That only works if the stack itself is defined correctly, which is covered in our guide to the Abaqus composite layup.

Element types that support Hashin

This is where a lot of models die before they start. Hashin damage in Abaqus requires a plane stress formulation. That means:

  • Conventional shells (S4R, S4, S3R)
  • Continuum shells (SC8R)
  • Plane stress elements (CPS4R)
  • Membranes (M3D4R)

It does not work with 3D solid elements such as C3D8R. If your laminate is meshed with solids, the Hashin option will not apply, and you need a user subroutine — a 3D Hashin VUMAT for Abaqus/Explicit or a UMAT for Abaqus/Standard. Fortran is the official language for Abaqus subroutines, so plan for that rather than assuming a C or C++ route.

If you are still deciding how to discretise the laminate, our guide on shell vs solid elements in FEA covers the trade-offs in more detail.

Setting it up, step by step

1. Orthotropic elasticity

In Abaqus/CAE: Property module → Material → Mechanical → Elasticity → Elastic → Type: Lamina. You supply E1, E2, Nu12, G12, G13 and G23. Using Engineering Constants instead will block the Hashin option, because that is a 3D definition.

2. Damage initiation — the six strengths

Mechanical → Damage for Fiber-Reinforced Composites → Hashin Damage. You enter six values, in this order:

  • Xt — longitudinal tensile strength
  • Xc — longitudinal compressive strength
  • Yt — transverse tensile strength
  • Yc — transverse compressive strength
  • Sl — longitudinal shear strength
  • St — transverse shear strength

An alpha coefficient controls how much shear stress contributes to the fibre tension criterion. The default of 0 gives the Hashin-Rotem form; 1 gives the full 1980 Hashin form. If you are matching a published paper, check which one it used.

3. Damage evolution — the four fracture energies

Right-click the Hashin damage definition and add the Damage Evolution suboption, type Energy, linear softening. You supply four fracture energies: Gft, Gfc, Gmt, Gmc.

In keyword form the whole material block looks like this:

*MATERIAL, NAME=CFRP
*ELASTIC, TYPE=LAMINA
 E1, E2, Nu12, G12, G13, G23
*DAMAGE INITIATION, CRITERION=HASHIN
 Xt, Xc, Yt, Yc, Sl, St
*DAMAGE EVOLUTION, TYPE=ENERGY, SOFTENING=LINEAR
 Gft, Gfc, Gmt, Gmc
*DAMAGE STABILIZATION
 v_ft, v_fc, v_mt, v_mc

4. Damage stabilization

In Abaqus/Standard, viscous regularization is usually the difference between a job that runs and a job that aborts. Add the Damage Stabilization suboption and give each of the four modes a small viscosity coefficient.

Start small — 1e-5 to 1e-4 is a reasonable first try for a quasi-static run — and treat anything larger as a red flag, because viscous regularization adds artificial strength. Always compare the damage stabilization energy (ALLCD) against the internal energy (ALLIE). More than a few percent means your peak load is partly fictional.

5. Element deletion

Element removal is controlled by section controls (*SECTION CONTROLS), with a maximum degradation value and deletion on or off. In Abaqus/Explicit this removes fully failed elements from the mesh. In Abaqus/Standard the element normally stays, stiffness capped at the degradation limit. This has changed between releases, so check the docs for your version.

6. Output you actually need

Request these, or you will not be able to explain your own results:

  • DAMAGEFT, DAMAGEFC, DAMAGEMT, DAMAGEMC — the four damage variables (0 to 1)
  • DMICRT — the initiation criteria (HSNFTCRT, HSNFCCRT, HSNMTCRT, HSNMCCRT); a value of 1 means that mode has initiated
  • SDEG — overall scalar stiffness degradation
  • STATUS — element status, needed if you are deleting elements

Where the fracture energies come from

This is the part nobody hands you. Strengths are usually on the datasheet. The four fracture energies almost never are.

Practical options, in order of preference:

  1. Published values for the same material system. IM7/8552 and T300/1034-C are well characterised in the literature and make a defensible starting point.
  2. Interlaminar values as an approximation. GIc from a DCB test is often used for Gmt, GIIc from an ENF test for Gmc. These are interlaminar properties standing in for intralaminar damage, so say so in your report.
  3. Calibration against a test curve. Fit the energies until the simulated load-displacement curve matches a coupon test.

One thing worth knowing before you start guessing: the fibre energies are two to three orders of magnitude larger than the matrix energies. For carbon/epoxy, Gft and Gfc are typically in the tens to low hundreds of N/mm, while Gmt is often below 1 N/mm. If your four numbers are all the same order, something is wrong.

Watch the units: N/mm equals kJ/m², but is a factor of 1000 from J/m². A model in mm/N/tonne needs energies in N/mm.

Mesh size still matters

Energy-based softening uses the element characteristic length to regularise the response. That removes most of the mesh dependence, but not all of it. If elements are too large, linear softening turns into snap-back and the solver cannot follow it. As a rough guideline for the fibre tension mode, keep the characteristic element length below about 2·E1·Gft / Xt², and always run two mesh densities before trusting a peak load.

Abaqus/Standard or Abaqus/Explicit?

Standard is fine up to and slightly past first failure. Once several elements soften at once it tends to stall, whatever you do to the increment size. For full progressive failure — impact, crushing, open-hole tension to collapse — Explicit is usually the better tool: load slowly with a smooth amplitude, keep kinetic energy below about 5% of internal energy, and use mass scaling carefully rather than aggressively.

Common mistakes

  • Initiation without evolution. Damage flags appear, stiffness never drops, load keeps rising.
  • Solid elements. The option is unavailable and people assume the model is broken.
  • Engineering Constants instead of Lamina. Same symptom, different cause.
  • Fracture energies off by 1000. Either nothing fails, or everything fails instantly.
  • Too much viscous regularization. The job converges beautifully and the peak load is wrong.
  • No damage output requested. You get a load drop and no way to say which mode caused it.
  • Expecting Hashin to predict delamination. It cannot — see below.

Hashin does not predict delamination

Hashin damage is intralaminar — damage inside a ply. Delamination is interlaminar — separation between plies. Different physics, different models.

For a realistic laminate under impact or bending you usually need both: Hashin in the plies, plus cohesive elements or surfaces at the interfaces. Our guide on simulating delamination growth with cohesive elements covers that side of the problem, and if you are comparing failure theories, the Tsai-Wu failure criterion guide explains why a single quadratic criterion tells you less than four separate modes.

Ready-to-use Abaqus models

If you would rather start from a model that already runs, these are the most relevant packages in our catalogue:

Frequently asked questions

Can I use Hashin damage with 3D solid elements in Abaqus?

No. The built-in Hashin model requires a plane stress formulation, so it works with shells, continuum shells, plane stress and membrane elements only. For 3D solids you need a 3D Hashin VUMAT (Explicit) or UMAT (Standard), written in Fortran.

What is the difference between Hashin damage and the Tsai-Wu criterion?

Tsai-Wu is a single quadratic criterion that tells you whether a ply has failed, with no information about how. Hashin separates fibre and matrix, tension and compression, into four modes, and each mode can degrade stiffness independently. Tsai-Wu is a check; Hashin is a progressive damage model.

Why does my Abaqus/Standard job stop right after damage starts?

Softening makes the tangent stiffness lose positive definiteness, and the implicit solver cannot follow it. Add damage stabilization with small viscosity coefficients, reduce the minimum increment size, and check ALLCD against ALLIE afterwards. If it still stalls, move the analysis to Abaqus/Explicit.

Where do I get Gft, Gfc, Gmt and Gmc?

Rarely from a datasheet. Use published values for the same material system, approximate the matrix energies from DCB and ENF interlaminar tests, or calibrate against a coupon test curve. Document whichever route you take — it is the largest source of uncertainty in the model.

Does Hashin damage predict delamination?

No. Hashin is intralaminar damage within a ply. Delamination is separation between plies and needs cohesive elements, cohesive surfaces, or VCCT at the interfaces.

Where to go next

Hashin damage stops being difficult once you see it as two definitions with two different jobs. Initiation is cheap and easy. Evolution is where the physics, the uncertainty and the convergence problems live — so spend your time on the fracture energies, the viscosity values and the mesh, not on the strengths.

For a working starting point, browse the composite and impact models in our shop. If you have a specific laminate, a test curve to match, or a model that will not get past first failure, we also take on custom simulation and consultation projects.

Reference: Abaqus documentation — Damage and failure for fiber-reinforced composites.

Leave a Reply

Your email address will not be published. Required fields are marked *

Related  articles

Abaqus Integration Point vs Nodal Stress: Why Peaks Differ
Compare integration-point, element-nodal and unique-nodal stress in Abaqus, and check whether a contour peak depends on extrapolation, averaging or mesh size.
Abaqus Linear Perturbation vs General Step: What Actually Changes
Abaqus Linear Perturbation vs General Step: What Actually Changes

You run a frequency extraction after a static step and the frequencies come out the same whether or not the part had yielded. You run a static linear perturbation step and the reaction force is a fraction of what you

Harmonic Response Analysis in ANSYS Workbench: A Practical Guide
Harmonic Response Analysis in ANSYS Workbench: A Practical Guide
How to set up harmonic response analysis in ANSYS Workbench: modal link, frequency range, solution method, damping, loads and results, plus the common mistakes.

See more

Related  Products

See more